</div>
<div>We have also experienced problems in our lab with Ni e-beam evaporation in VC or Al2O3 crucibles.  We found that the VC crucibles would break down after a few deposition cycles (and would “tarnish” the Ni melt) and the one time we tried Al2O3 as a crucible
 liner it broke immediately upon removal from our E-beam hearth.  We have settled on using Tungsten crucibles for our Ni e-beam evaporation.  We have not observed any notable problems with this process and our first W crucible lasted for over two years before
 we needed to retire it.</div>
<div><br>
</div>
<div>Best regards,</div>
<div>  -Nathan</div>
<div>
<div>-- </div>
<div>Nathan Nelson-Fitzpatrick  PhD</div>
<div>Nanofabrication Process Engineer</div>
<div>Quantum NanoFab</div>
<div>University of Waterloo</div>
<div>200 University Avenue West</div>
<div>Waterloo, ON   Canada  N2L 3G1</div>
<div>Ph: +1 519-888-4567 ext. 31796</div>
<div><br>
</div>
<div><span class="Apple-style-span" style="border-collapse: collapse; color: rgb(80, 0, 80);">
<p class="MsoNormal" style="font-size: 11pt; font-family: Calibri, sans-serif;"><br>
</p>
<span class="Apple-style-span" style="font-size: 15px;"><br>
</span>
<p class="MsoNormal" style="font-size: 11pt; font-family: Calibri, sans-serif;"><br>
</p>
</span></div>
</div>
</div>
<div><br>
</div>
<span id="OLK_SRC_BODY_SECTION">
<div style="font-family:Calibri; font-size:11pt; text-align:left; color:black; BORDER-BOTTOM: medium none; BORDER-LEFT: medium none; PADDING-BOTTOM: 0in; PADDING-LEFT: 0in; PADDING-RIGHT: 0in; BORDER-TOP: #b5c4df 1pt solid; BORDER-RIGHT: medium none; PADDING-TOP: 3pt">
<span style="font-weight:bold">From: </span>Nava Ariel- Sternberg <<a href="mailto:anava@tauex.tau.ac.il">anava@tauex.tau.ac.il</a>><br>
<span style="font-weight:bold">Date: </span>Monday, March 23, 2015 at 5:30 AM<br>
<span style="font-weight:bold">To: </span>"<a href="mailto:labnetwork@mtl.mit.edu">labnetwork@mtl.mit.edu</a>" <<a href="mailto:labnetwork@mtl.mit.edu">labnetwork@mtl.mit.edu</a>><br>
<span style="font-weight:bold">Subject: </span>[labnetwork] Ni evaporation<br>
</div>
<div><br>
</div>
<div xmlns:v="urn:schemas-microsoft-com:vml" xmlns:o="urn:schemas-microsoft-com:office:office" xmlns:w="urn:schemas-microsoft-com:office:word" xmlns:m="http://schemas.microsoft.com/office/2004/12/omml" xmlns="http://www.w3.org/TR/REC-html40">
<meta name="Generator" content="Microsoft Word 14 (filtered medium)">
<style><!--
/* Font Definitions */
@font-face
        {font-family:Calibri;
        panose-1:2 15 5 2 2 2 4 3 2 4;}
@font-face
        {font-family:Consolas;
        panose-1:2 11 6 9 2 2 4 3 2 4;}
/* Style Definitions */
p.MsoNormal, li.MsoNormal, div.MsoNormal
        {margin:0cm;
        margin-bottom:.0001pt;
        font-size:12.0pt;
        font-family:"Times New Roman","serif";
        color:black;}
a:link, span.MsoHyperlink
        {mso-style-priority:99;
        color:blue;
        text-decoration:underline;}
a:visited, span.MsoHyperlinkFollowed
        {mso-style-priority:99;
        color:purple;
        text-decoration:underline;}
pre
        {mso-style-priority:99;
        mso-style-link:"HTML Preformatted Char";
        margin:0cm;
        margin-bottom:.0001pt;
        font-size:10.0pt;
        font-family:"Courier New";
        color:black;}
span.HTMLPreformattedChar
        {mso-style-name:"HTML Preformatted Char";
        mso-style-priority:99;
        mso-style-link:"HTML Preformatted";
        font-family:Consolas;
        color:black;}
span.EmailStyle19
        {mso-style-type:personal-reply;
        font-family:"Calibri","sans-serif";
        color:#1F497D;}
.MsoChpDefault
        {mso-style-type:export-only;
        font-size:10.0pt;}
@page WordSection1
        {size:612.0pt 792.0pt;
        margin:72.0pt 90.0pt 72.0pt 90.0pt;}
div.WordSection1
        {page:WordSection1;}
--></style><!--[if gte mso 9]><xml>
<o:shapedefaults v:ext="edit" spidmax="1026" />
</xml><![endif]--><!--[if gte mso 9]><xml>
<o:shapelayout v:ext="edit">
<o:idmap v:ext="edit" data="1" />
</o:shapelayout></xml><![endif]-->
<div bgcolor="white" lang="EN-US" link="blue" vlink="purple">
<div class="WordSection1">
<p class="MsoNormal"><span style="font-size: 11pt; font-family: Calibri, sans-serif; color: rgb(31, 73, 125);">Hi all,<o:p></o:p></span></p>
<p class="MsoNormal"><span style="font-size: 11pt; font-family: Calibri, sans-serif; color: rgb(31, 73, 125);"><o:p> </o:p></span></p>
<p class="MsoNormal"><span style="font-size: 11pt; font-family: Calibri, sans-serif; color: rgb(31, 73, 125);">We've came across some issues with Ni e-beam evaporation and thought of consulting the network:<o:p></o:p></span></p>
<p class="MsoNormal"><span style="font-size: 11pt; font-family: Calibri, sans-serif; color: rgb(31, 73, 125);"><o:p> </o:p></span></p>
<p class="MsoNormal"><span style="font-size: 11pt; font-family: Calibri, sans-serif; color: rgb(31, 73, 125);">Which crucible are you using for Ni e-beam evaporation? We've tried Al2O3 and Vitreous carbon, both recommended by the material/crucible suppliers.<o:p></o:p></span></p>
<p class="MsoNormal"><span style="font-size: 11pt; font-family: Calibri, sans-serif; color: rgb(31, 73, 125);">Any tips with respect to melting the material or the evaporation process itself?
<o:p></o:p></span></p>
<p class="MsoNormal"><span style="font-size: 11pt; font-family: Calibri, sans-serif; color: rgb(31, 73, 125);"><o:p> </o:p></span></p>
<p class="MsoNormal"><span style="font-size: 11pt; font-family: Calibri, sans-serif; color: rgb(31, 73, 125);">Thanks,<o:p></o:p></span></p>
<p class="MsoNormal"><span style="font-size: 11pt; font-family: Calibri, sans-serif; color: rgb(31, 73, 125);"><o:p> </o:p></span></p>
<p class="MsoNormal"><span style="font-size: 11pt; font-family: Calibri, sans-serif; color: rgb(31, 73, 125);">Nava<o:p></o:p></span></p>
<p class="MsoNormal"><span style="font-size: 11pt; font-family: Calibri, sans-serif; color: rgb(31, 73, 125);"><o:p> </o:p></span></p>
<div>
<p class="MsoNormal"><span style="font-size: 11pt; font-family: Calibri, sans-serif; color: rgb(31, 73, 125);"><o:p> </o:p></span></p>
<p class="MsoNormal"><span style="font-size: 11pt; font-family: Calibri, sans-serif; color: rgb(31, 73, 125);">Nava Ariel-Sternberg, Ph.D.<o:p></o:p></span></p>
<p class="MsoNormal"><span style="font-size: 11pt; font-family: Calibri, sans-serif; color: rgb(31, 73, 125);">Tel-Aviv University Center for Nanoscience and Nanotechnology, Managing Director<o:p></o:p></span></p>
<p class="MsoNormal"><span style="font-size: 11pt; font-family: Calibri, sans-serif; color: rgb(31, 73, 125);">MNCF Manager<o:p></o:p></span></p>
<p class="MsoNormal"><span style="font-size: 11pt; font-family: Calibri, sans-serif; color: rgb(31, 73, 125);">Phone: 03-640-5619</span><span lang="HE" dir="RTL" style="font-size: 11pt; font-family: Arial, sans-serif; color: rgb(31, 73, 125);"><o:p></o:p></span></p>
<p class="MsoNormal"><span style="font-size: 11pt; font-family: Calibri, sans-serif; color: rgb(31, 73, 125);">Mobile: 054-9984959<o:p></o:p></span></p>
<p class="MsoNormal"><span style="font-size: 11pt; font-family: Calibri, sans-serif; color: rgb(31, 73, 125);">Email:
<a href="mailto:anava@tauex.tau.ac.il"><span style="color:blue">anava@tauex.tau.ac.il</span></a><o:p></o:p></span></p>
</div>
<p class="MsoNormal"><span style="font-size: 11pt; font-family: Calibri, sans-serif; color: rgb(31, 73, 125);"><o:p> </o:p></span></p>
</div>
</div>
</div>
</span>
</body>
</html>