<div dir="ltr">Another downside (besdies cost) is Au sticks to W - not a big problem for most.<div>-Hal</div><div> </div></div><div class="gmail_extra"><br><div class="gmail_quote">On Sat, Jul 23, 2016 at 3:09 PM, Michael Rooks <span dir="ltr"><<a href="mailto:michael.rooks@yale.edu" target="_blank">michael.rooks@yale.edu</a>></span> wrote:<br><blockquote class="gmail_quote" style="margin:0 0 0 .8ex;border-left:1px #ccc solid;padding-left:1ex">
<div bgcolor="#FFFFFF" text="#000000">
<p>Matt is right. It is well known that gold will form clumps around
carbon particles. It's easy to evaporate some of the carbon
crucible accidentally, and so it's important to use either Mo or W
crucibles. Either type of crucible will cost a lot less than the
gold you put in it. By the way, you'll have to throw out the
contaminated gold. <br>
</p>
<div><br>
<font size="-2">----------------------------------<br>
Michael Rooks
<br>
Yale Institute of Nanoscience and Quantum Engineering
<br>
<a href="http://nano.yale.edu" target="_blank">nano.yale.edu</a>
</font>
<br>
<br>
<br>
<br>
</div>
<div>On 7/23/16 11:40 AM, Matt Moneck wrote:<br>
</div>
<blockquote type="cite">
<pre>Hi Sunanda,
We had similar issues in the past with a Fabmate (i.e. graphite) crucible.
We had the same gold nodules on the side of the crucible and we had similar
"bubbles" in some of our films. We also saw carbon residue on the Au
charge. After discussing with some companies, our Process Engineer prompted
the switch to a tungsten crucible and it solved all of our problems. The
bubbles and nodules went away, and the the sheet resistance of our films
improved. Tungsten is more expensive, but it is worth it in my opinion.
Best Regards,
Matt
</pre>
</blockquote>
<br>
</div>
<br>_______________________________________________<br>
labnetwork mailing list<br>
<a href="mailto:labnetwork@mtl.mit.edu">labnetwork@mtl.mit.edu</a><br>
<a href="https://www-mtl.mit.edu/mailman/listinfo.cgi/labnetwork" rel="noreferrer" target="_blank">https://www-mtl.mit.edu/mailman/listinfo.cgi/labnetwork</a><br>
<br></blockquote></div><br></div>