<div>HI, Paul, </div>
<div>We in CNS evaluated different chambers and ICP systems for LiNbO3 etching, and it turned out Ulvac ICP NLD-570 gave us better results.  Instead of fluorine, we just used Ar (physical sputtering). Redeposition is always an issue for LiNbO3 etching, and
 it is critical to tune the power, pressure and temperature.  This etching process/recipe have been used for LiNbO3 high speed modulator application for about 2 years (please check Prof. Marko Loncar group's recent publication).  </div>
<div>Our ULVAC NLD-570 RIE is dedicated for oxide material etching, we haven’t seen too much impact to the SiO2, SiN etching. We have different chamber for Si device process. the tool is relative new (2 years old), we just opened the chamber for deep PM once. </div>
<div>Please feel free to contact us (Kenlin- cced and myself) if you need more detailed information…</div>
<div><br>
</div>
<div>Best!</div>
<div><br>
</div>
<div><br>
</div>
<div>-JD </div>
<div><br>
</div>
<div><br>
</div>
<div>
<div>-- Jiangdong Deng (JD), Ph.D,</div>
<div><br>
</div>
<div>Associate Director</div>
<div>Senior Principal Scientist,</div>
<div>Center for Nanoscale Systems, </div>
<div>Head of Nanofabrication Facility</div>
<div>Harvard University, </div>
<div>Cambridge, MA 02138</div>
<div>Tel: 617-495-3396</div>
<div><br>
</div>
</div>
<div>     </div>
<div><br>
</div>
<span id="OLK_SRC_BODY_SECTION">
<div style="font-family:Calibri; font-size:11pt; text-align:left; color:black; BORDER-BOTTOM: medium none; BORDER-LEFT: medium none; PADDING-BOTTOM: 0in; PADDING-LEFT: 0in; PADDING-RIGHT: 0in; BORDER-TOP: #b5c4df 1pt solid; BORDER-RIGHT: medium none; PADDING-TOP: 3pt">
<span style="font-weight:bold">From: </span><<a href="mailto:labnetwork-bounces@mtl.mit.edu">labnetwork-bounces@mtl.mit.edu</a>> on behalf of "<a href="mailto:patricns@uw.edu">patricns@uw.edu</a>" <<a href="mailto:patricns@uw.edu">patricns@uw.edu</a>><br>
<span style="font-weight:bold">Date: </span>Thursday, January 18, 2018 at 4:57 PM<br>
<span style="font-weight:bold">To: </span>"Horng, Paul S." <<a href="mailto:horng@udel.edu">horng@udel.edu</a>><br>
<span style="font-weight:bold">Cc: </span>"labnetwork@mtl. Network" <<a href="mailto:labnetwork@mtl.mit.edu">labnetwork@mtl.mit.edu</a>><br>
<span style="font-weight:bold">Subject: </span>Re: [labnetwork] ICP etch of LiNbO3<br>
</div>
<div><br>
</div>
<div>
<div style="word-wrap: break-word; -webkit-nbsp-mode: space; -webkit-line-break: after-white-space;" class="">
Hello Paul,
<div class=""><br class="">
</div>
<div class="">We’ve had some experience now with lithium niobate materials in an Oxford Plasmalab 100 ICP tool using fluorine chemistry. The problem we have found is that the by-products are not truly volatile and tend to deposit on everything where they are,
 in subsequent processes, likely to to be etched and redeposited.</div>
<div class=""><br class="">
</div>
<div class="">This has lead to micro masking, deposition on other substrates where it is not ideal, and plasma loading to the point of significant degradation of etch rates and uniformity. because of this, we were forced to do a hard, open chamber scrub and
 clean each time this process was run, followed by a few etch and clean cycles to get mostly back to normal operation. The maintenance time is such that I recommend staying away form this process if at all possible.</div>
<div class=""><br class="">
</div>
<div class="">We’ve not seen a negative effect on ultimate vacuum pressure or pump lifetime, but we’ve also reduced the frequency at which we allow this process due to the cleaning involved, so it may be we just haven’t had enough material go through to truly
 evaluate pump performance and lifetime expectancy.</div>
<div class=""><br class="">
</div>
<div class="">Best of luck. If you’d like more information on what we’ve seen, let me know and I’ll put you in contact with our etch engineer who has been attempting to cope with the matter.</div>
<div class=""><br class="">
</div>
<div class="">
<div class="">
<div style="color: rgb(0, 0, 0); letter-spacing: normal; orphans: auto; text-align: start; text-indent: 0px; text-transform: none; white-space: normal; widows: auto; word-spacing: 0px; -webkit-text-stroke-width: 0px; word-wrap: break-word; -webkit-nbsp-mode: space; -webkit-line-break: after-white-space;" class="">
<div style="color: rgb(0, 0, 0); letter-spacing: normal; orphans: auto; text-align: start; text-indent: 0px; text-transform: none; white-space: normal; widows: auto; word-spacing: 0px; -webkit-text-stroke-width: 0px; word-wrap: break-word; -webkit-nbsp-mode: space; -webkit-line-break: after-white-space;" class="">
<div style="color: rgb(0, 0, 0); letter-spacing: normal; orphans: auto; text-align: start; text-indent: 0px; text-transform: none; white-space: normal; widows: auto; word-spacing: 0px; -webkit-text-stroke-width: 0px; word-wrap: break-word; -webkit-nbsp-mode: space; -webkit-line-break: after-white-space;" class="">
<div style="color: rgb(0, 0, 0); letter-spacing: normal; orphans: auto; text-align: start; text-indent: 0px; text-transform: none; white-space: normal; widows: auto; word-spacing: 0px; -webkit-text-stroke-width: 0px; word-wrap: break-word; -webkit-nbsp-mode: space; -webkit-line-break: after-white-space;" class="">
<div class="">
<div class="">N. Shane Patrick<br class="">
Research Engineer, Washington Nanofabrication Facility (WNF) <br class="">
National Nanotechnology Coordinated Infrastructure (NNCI)<br class="">
University of Washington<br class="">
Fluke Hall 132, Box 352143</div>
<div class="">(206) 221-1045</div>
<div class=""><a href="mailto:patricns@uw.edu" class="">patricns@uw.edu</a></div>
<div class=""><a href="http://www.wnf.washington.edu/" class="">http://www.wnf.washington.edu/</a></div>
</div>
</div>
</div>
</div>
</div>
</div>
<br class="">
<div>
<blockquote type="cite" class="">
<div class="">On Jan 18, 2018, at 11:28 AM, Horng, Paul S. <<a href="mailto:horng@udel.edu" class="">horng@udel.edu</a>> wrote:</div>
<br class="Apple-interchange-newline">
<div class="">
<div class="WordSection1" style="page: WordSection1; font-family: Helvetica; font-size: 12px; font-style: normal; font-variant-caps: normal; font-weight: normal; letter-spacing: normal; text-align: start; text-indent: 0px; text-transform: none; white-space: normal; word-spacing: 0px; -webkit-text-stroke-width: 0px;">
<div style="margin: 0in 0in 0.0001pt; font-size: 11pt; font-family: Calibri, sans-serif;" class="">
Hi,<o:p class=""></o:p></div>
<div style="margin: 0in 0in 0.0001pt; font-size: 11pt; font-family: Calibri, sans-serif;" class="">
Has anyone had experience with plasma etching of LiNbO3 films ? It is hard to etch so higher platen power is needed to enhance physical sputtering. What is the impact on etch rate of other processes like etching of Si, SiO2, SiN, etc. in the same chamber ?
  How often is chamber liner needed to be scrubbed clean ? Will it shorten the life of turbo pump ?    <o:p class=""></o:p></div>
<div style="margin: 0in 0in 0.0001pt; font-size: 11pt; font-family: Calibri, sans-serif;" class="">
<o:p class=""> </o:p></div>
<div style="margin: 0in 0in 0.0001pt; font-size: 11pt; font-family: Calibri, sans-serif;" class="">
Thank You,<o:p class=""></o:p></div>
<div style="margin: 0in 0in 0.0001pt; font-size: 11pt; font-family: Calibri, sans-serif;" class="">
<o:p class=""> </o:p></div>
<div style="margin: 0in 0in 0.0001pt; font-size: 11pt; font-family: Calibri, sans-serif;" class="">
Paul S. Horng, Ph.D<o:p class=""></o:p></div>
<div style="margin: 0in 0in 0.0001pt; font-size: 11pt; font-family: Calibri, sans-serif;" class="">
Process Engineer, UD NanoFab<o:p class=""></o:p></div>
<div style="margin: 0in 0in 0.0001pt; font-size: 11pt; font-family: Calibri, sans-serif;" class="">
457 ISE Lab<o:p class=""></o:p></div>
<div style="margin: 0in 0in 0.0001pt; font-size: 11pt; font-family: Calibri, sans-serif;" class="">
221 Academy Street, Newark, DE 19716<o:p class=""></o:p></div>
<div style="margin: 0in 0in 0.0001pt; font-size: 11pt; font-family: Calibri, sans-serif;" class="">
(302)831-4827<o:p class=""></o:p></div>
<div style="margin: 0in 0in 0.0001pt; font-size: 11pt; font-family: Calibri, sans-serif;" class="">
<a href="http://udnf.udel.edu/" style="color: rgb(149, 79, 114); text-decoration: underline;" class="">http://udnf.udel.edu</a><o:p class=""></o:p></div>
<div style="margin: 0in 0in 0.0001pt; font-size: 11pt; font-family: Calibri, sans-serif;" class="">
<o:p class=""> </o:p></div>
</div>
<span style="font-family: Helvetica; font-size: 12px; font-style: normal; font-variant-caps: normal; font-weight: normal; letter-spacing: normal; text-align: start; text-indent: 0px; text-transform: none; white-space: normal; word-spacing: 0px; -webkit-text-stroke-width: 0px; float: none; display: inline !important;" class="">_______________________________________________</span><br style="font-family: Helvetica; font-size: 12px; font-style: normal; font-variant-caps: normal; font-weight: normal; letter-spacing: normal; text-align: start; text-indent: 0px; text-transform: none; white-space: normal; word-spacing: 0px; -webkit-text-stroke-width: 0px;" class="">
<span style="font-family: Helvetica; font-size: 12px; font-style: normal; font-variant-caps: normal; font-weight: normal; letter-spacing: normal; text-align: start; text-indent: 0px; text-transform: none; white-space: normal; word-spacing: 0px; -webkit-text-stroke-width: 0px; float: none; display: inline !important;" class="">labnetwork
 mailing list</span><br style="font-family: Helvetica; font-size: 12px; font-style: normal; font-variant-caps: normal; font-weight: normal; letter-spacing: normal; text-align: start; text-indent: 0px; text-transform: none; white-space: normal; word-spacing: 0px; -webkit-text-stroke-width: 0px;" class="">
<a href="mailto:labnetwork@mtl.mit.edu" style="color: rgb(149, 79, 114); text-decoration: underline; font-family: Helvetica; font-size: 12px; font-style: normal; font-variant-caps: normal; font-weight: normal; letter-spacing: normal; orphans: auto; text-align: start; text-indent: 0px; text-transform: none; white-space: normal; widows: auto; word-spacing: 0px; -webkit-text-size-adjust: auto; -webkit-text-stroke-width: 0px;" class="">labnetwork@mtl.mit.edu</a><br style="font-family: Helvetica; font-size: 12px; font-style: normal; font-variant-caps: normal; font-weight: normal; letter-spacing: normal; text-align: start; text-indent: 0px; text-transform: none; white-space: normal; word-spacing: 0px; -webkit-text-stroke-width: 0px;" class="">
<a href="https://mtl.mit.edu/mailman/listinfo.cgi/labnetwork" style="color: rgb(149, 79, 114); text-decoration: underline; font-family: Helvetica; font-size: 12px; font-style: normal; font-variant-caps: normal; font-weight: normal; letter-spacing: normal; orphans: auto; text-align: start; text-indent: 0px; text-transform: none; white-space: normal; widows: auto; word-spacing: 0px; -webkit-text-size-adjust: auto; -webkit-text-stroke-width: 0px;" class="">https://mtl.mit.edu/mailman/listinfo.cgi/labnetwork</a></div>
</blockquote>
</div>
<br class="">
</div>
</div>
</div>
</span>
</body>
</html>