<div>In my haste to write something up and get out the door I mixed up the gas is in the problem description.</div>
<div><span style="background-color: rgba(255, 255, 255, 0);"><br>
</span></div>
<div><span style="background-color: rgba(255, 255, 255, 0);">Our process is typical Bosch SF6 and O2 for etching .... switching off with C4F8 for passivation...</span></div>
<div><span style="background-color: rgba(255, 255, 255, 0);"><br>
</span></div>
<div><span style="background-color: rgba(255, 255, 255, 0);">Mark</span></div>
<div><br>
<div id="AppleMailSignature" dir="ltr"><span style="background-color: rgba(255, 255, 255, 0);"><b>Mark Weiler</b><br>
Equipment & Facilities Manager</span>
<div><span style="background-color: rgba(255, 255, 255, 0);">Claire and John Bertucci Nanotechnology Laboratory<br>
Electrical and Computer Engineering | Carnegie Mellon University<br>
<a href="x-apple-data-detectors://3/1" dir="ltr" x-apple-data-detectors="true" x-apple-data-detectors-type="address" x-apple-data-detectors-result="3/1" style="-webkit-text-decoration-color: rgba(33, 33, 33, 0.258824);">5000 Forbes Ave., Pittsburgh, PA 15213-3890</a><br>
T: <a href="tel:412.268.5430" dir="ltr" x-apple-data-detectors="true" x-apple-data-detectors-type="telephone" x-apple-data-detectors-result="3/2" style="-webkit-text-decoration-color: rgba(33, 33, 33, 0.258824);">412.268.2471</a><br>
F: <a href="tel:412.268.3497" dir="ltr" x-apple-data-detectors="true" x-apple-data-detectors-type="telephone" x-apple-data-detectors-result="3/3" style="-webkit-text-decoration-color: rgba(33, 33, 33, 0.258824);">412.268.3497</a><br>
<a href="http://www.ece.cmu.edu/">www.ece.cmu.edu</a><br>
<a href="http://nanofab.ece.cmu.edu/" dir="ltr" x-apple-data-detectors="true" x-apple-data-detectors-type="link" x-apple-data-detectors-result="4">nanofab.ece.cmu.edu</a></span></div>
</div>
<div dir="ltr"><br>
On Mar 5, 2019, at 18:42, Mark Weiler <<a href="mailto:mweiler@andrew.cmu.edu">mweiler@andrew.cmu.edu</a>> wrote:<br>
<br>
</div>
<blockquote type="cite">
<div dir="ltr">Hello Everyone,
<div class=""><br class="">
</div>
<div class="">We have gone through seven new lip seals purchased form Orbotech/SPTS. They are often failing before we even finish qualifying the system, or within a month thereafter.
<div class=""><br class="">
</div>
<div class="">Our our process is stable with power and parameters not deviating over the past decade. However, I ordered the most recent batch of lip seals because the wafer seals we had been using were coming out with black residue after only a few runs…
however, the current ones do the same. Not only have the lips seals disintegrated, but the chamber lid o-ring and bottom ceramic spool o-ring have also failed with black rubber material shedding off. It’s as if they are made of Buna and not meant for this
application.</div>
<div class=""><br class="">
</div>
<div class="">Our process is typical Bosch with 100 sccm C4F8 and 20 sccm O2 for etching switching off with ~50 Sccm SF6 for passivation at a processing pressure of 15 mTorr, Coil power 600-800W, Platen power 100-150W, Bias voltage 50-100v (up to 200 peak-to-peak),
Platen temp at 19 degrees, Lid temp 41 degrees. Qual wafers are new bare Silicon. Etch rates are normal and stable with 10+ years of data…. we just can’t complete the work due to failing seals.</div>
<div class=""><br class="">
</div>
<div class="">Our chamber base pressure is between 1E-8 and 5E-8 Torr each morning. When we put in a brand new seal and run only the LUR, it passes with 0.00 mTorr/minute leak rate. That jumps to 3.00 mTorr/m after only 30 minutes of the SPTS recommended
O2 Clean… then rises as time and more runs progress. Wafers are coming out with black rings on their backsides. </div>
<div class=""><br class="">
</div>
<div class="">This should not be happening, and I believe it is due to incorrect material of the lip seals and o-rings. I am pinging the network, though, to see if there might be a parameter change we need to effect that may assist us.</div>
<div class=""><br class="">
</div>
<div class="">Have any of you seen this before?</div>
<div class=""><br class="">
</div>
<div class="">Best regards,</div>
<div class=""><br class="">
</div>
<div class="">Mark</div>
<div class="">
<div style="caret-color: rgb(0, 0, 0); color: rgb(0, 0, 0); font-family: Helvetica; font-size: 12px; font-style: normal; font-variant-caps: normal; font-weight: normal; letter-spacing: normal; orphans: auto; text-align: start; text-indent: 0px; text-transform: none; white-space: normal; widows: auto; word-spacing: 0px; -webkit-text-size-adjust: auto; -webkit-text-stroke-width: 0px; text-decoration: none; font-variant-ligatures: normal; font-variant-position: normal; font-variant-numeric: normal; font-variant-alternates: normal; font-variant-east-asian: normal;" class="">
<br class="Apple-interchange-newline">
<br class="">
</div>
<div style="caret-color: rgb(0, 0, 0); color: rgb(0, 0, 0); font-family: Helvetica; font-size: 12px; font-style: normal; font-variant-caps: normal; font-weight: normal; letter-spacing: normal; orphans: auto; text-align: start; text-indent: 0px; text-transform: none; white-space: normal; widows: auto; word-spacing: 0px; -webkit-text-size-adjust: auto; -webkit-text-stroke-width: 0px; text-decoration: none; font-variant-ligatures: normal; font-variant-position: normal; font-variant-numeric: normal; font-variant-alternates: normal; font-variant-east-asian: normal;" class="">
________________________________________________________________</div>
<div style="caret-color: rgb(0, 0, 0); color: rgb(0, 0, 0); font-family: Helvetica; font-size: 12px; font-style: normal; font-variant-caps: normal; font-weight: normal; letter-spacing: normal; orphans: auto; text-align: start; text-indent: 0px; text-transform: none; white-space: normal; widows: auto; word-spacing: 0px; -webkit-text-size-adjust: auto; -webkit-text-stroke-width: 0px; text-decoration: none; font-variant-ligatures: normal; font-variant-position: normal; font-variant-numeric: normal; font-variant-alternates: normal; font-variant-east-asian: normal;" class="">
<br class="">
</div>
<div style="caret-color: rgb(0, 0, 0); color: rgb(0, 0, 0); font-family: Helvetica; font-size: 12px; font-style: normal; font-variant-caps: normal; font-weight: normal; letter-spacing: normal; orphans: auto; text-align: start; text-indent: 0px; text-transform: none; white-space: normal; widows: auto; word-spacing: 0px; -webkit-text-size-adjust: auto; -webkit-text-stroke-width: 0px; text-decoration: none; font-variant-ligatures: normal; font-variant-position: normal; font-variant-numeric: normal; font-variant-alternates: normal; font-variant-east-asian: normal;" class="">
Mark Weiler</div>
<div style="caret-color: rgb(0, 0, 0); color: rgb(0, 0, 0); font-family: Helvetica; font-size: 12px; font-style: normal; font-variant-caps: normal; font-weight: normal; letter-spacing: normal; orphans: auto; text-align: start; text-indent: 0px; text-transform: none; white-space: normal; widows: auto; word-spacing: 0px; -webkit-text-size-adjust: auto; -webkit-text-stroke-width: 0px; text-decoration: none; font-variant-ligatures: normal; font-variant-position: normal; font-variant-numeric: normal; font-variant-alternates: normal; font-variant-east-asian: normal;" class="">
Equipment & Facilites Manager</div>
<div style="caret-color: rgb(0, 0, 0); color: rgb(0, 0, 0); font-family: Helvetica; font-size: 12px; font-style: normal; font-variant-caps: normal; font-weight: normal; letter-spacing: normal; orphans: auto; text-align: start; text-indent: 0px; text-transform: none; white-space: normal; widows: auto; word-spacing: 0px; -webkit-text-size-adjust: auto; -webkit-text-stroke-width: 0px; text-decoration: none; font-variant-ligatures: normal; font-variant-position: normal; font-variant-numeric: normal; font-variant-alternates: normal; font-variant-east-asian: normal;" class="">
Clair and John Bertucci Nanotechnology Laboratory</div>
<div style="caret-color: rgb(0, 0, 0); color: rgb(0, 0, 0); font-family: Helvetica; font-size: 12px; font-style: normal; font-variant-caps: normal; font-weight: normal; letter-spacing: normal; orphans: auto; text-align: start; text-indent: 0px; text-transform: none; white-space: normal; widows: auto; word-spacing: 0px; -webkit-text-size-adjust: auto; -webkit-text-stroke-width: 0px; text-decoration: none; font-variant-ligatures: normal; font-variant-position: normal; font-variant-numeric: normal; font-variant-alternates: normal; font-variant-east-asian: normal;" class="">
Eden Hall Nanofabrication Cleanroom</div>
<div style="caret-color: rgb(0, 0, 0); color: rgb(0, 0, 0); font-family: Helvetica; font-size: 12px; font-style: normal; font-variant-caps: normal; font-weight: normal; letter-spacing: normal; orphans: auto; text-align: start; text-indent: 0px; text-transform: none; white-space: normal; widows: auto; word-spacing: 0px; -webkit-text-size-adjust: auto; -webkit-text-stroke-width: 0px; text-decoration: none; font-variant-ligatures: normal; font-variant-position: normal; font-variant-numeric: normal; font-variant-alternates: normal; font-variant-east-asian: normal;" class="">
Carnegie Mellon University</div>
<div style="caret-color: rgb(0, 0, 0); color: rgb(0, 0, 0); font-family: Helvetica; font-size: 12px; font-style: normal; font-variant-caps: normal; font-weight: normal; letter-spacing: normal; orphans: auto; text-align: start; text-indent: 0px; text-transform: none; white-space: normal; widows: auto; word-spacing: 0px; -webkit-text-size-adjust: auto; -webkit-text-stroke-width: 0px; text-decoration: none; font-variant-ligatures: normal; font-variant-position: normal; font-variant-numeric: normal; font-variant-alternates: normal; font-variant-east-asian: normal;" class="">
P: 412-268-2471</div>
<div style="caret-color: rgb(0, 0, 0); color: rgb(0, 0, 0); font-family: Helvetica; font-size: 12px; font-style: normal; font-variant-caps: normal; font-weight: normal; letter-spacing: normal; orphans: auto; text-align: start; text-indent: 0px; text-transform: none; white-space: normal; widows: auto; word-spacing: 0px; -webkit-text-size-adjust: auto; -webkit-text-stroke-width: 0px; text-decoration: none; font-variant-ligatures: normal; font-variant-position: normal; font-variant-numeric: normal; font-variant-alternates: normal; font-variant-east-asian: normal;" class="">
<a href="http://www.nanofab.ece.cmu.edu" class="">http://www.nanofab.ece.cmu.edu</a></div>
<div style="caret-color: rgb(0, 0, 0); color: rgb(0, 0, 0); font-family: Helvetica; font-size: 12px; font-style: normal; font-variant-caps: normal; font-weight: normal; letter-spacing: normal; orphans: auto; text-align: start; text-indent: 0px; text-transform: none; white-space: normal; widows: auto; word-spacing: 0px; -webkit-text-size-adjust: auto; -webkit-text-stroke-width: 0px; text-decoration: none; font-variant-ligatures: normal; font-variant-position: normal; font-variant-numeric: normal; font-variant-alternates: normal; font-variant-east-asian: normal;" class="">
<br class="">
</div>
<br class="Apple-interchange-newline" style="caret-color: rgb(0, 0, 0); color: rgb(0, 0, 0); font-family: Helvetica; font-size: 12px; font-style: normal; font-variant-caps: normal; font-weight: normal; letter-spacing: normal; orphans: auto; text-align: start; text-indent: 0px; text-transform: none; white-space: normal; widows: auto; word-spacing: 0px; -webkit-text-size-adjust: auto; -webkit-text-stroke-width: 0px; text-decoration: none;">
<a href="https://www.linkedin.com/in/marksbasics" style="font-family: Helvetica; font-size: 12px; font-style: normal; font-variant-caps: normal; font-weight: normal; letter-spacing: normal; orphans: auto; text-align: start; text-indent: 0px; text-transform: none; white-space: normal; widows: auto; word-spacing: 0px; -webkit-text-size-adjust: auto; -webkit-text-stroke-width: 0px;" class=""><span><span><span><span><span><span><img apple-inline="yes" id="907B832A-B6D1-4755-A3EC-AF5A9FDA77D6" src="cid:2D2E01E3-CEC1-4F48-A845-224D8D7CED12@wv.cc.cmu.edu"></span>
</span></span></span></span></span></a></div>
<a href="https://www.linkedin.com/in/marksbasics" style="font-family: Helvetica; font-size: 12px; font-style: normal; font-variant-caps: normal; font-weight: normal; letter-spacing: normal; orphans: auto; text-align: start; text-indent: 0px; text-transform: none; white-space: normal; widows: auto; word-spacing: 0px; -webkit-text-size-adjust: auto; -webkit-text-stroke-width: 0px;" class=""></a><br class="">
</div>
</div>
</blockquote>
<blockquote type="cite">
<div dir="ltr"><span>_______________________________________________</span><br>
<span>labnetwork mailing list</span><br>
<span><a href="mailto:labnetwork@mtl.mit.edu">labnetwork@mtl.mit.edu</a></span><br>
<span><a href="https://mtl.mit.edu/mailman/listinfo.cgi/labnetwork">https://mtl.mit.edu/mailman/listinfo.cgi/labnetwork</a></span><br>
</div>
</blockquote>
</div>
</body>
</html>