    <p>We use a Cu crucible (4.4cc in a 7cc pocket) with good results.</p>
    <p>Mario</p>
    <p><br>
    </p>
    <p></p>
    <div class="moz-cite-prefix">On 2024-12-11 9:11 a.m., Graham Gibson
      wrote:<br>
    </div>
    <blockquote type="cite"
cite="mid:TO1PPF1B624A34D95DBAC784BF3D6F5D280C33E2@TO1PPF1B624A34D.CANPRD01.PROD.OUTLOOK.COM">
      <meta http-equiv="Content-Type" content="text/html; charset=UTF-8">
      <meta name="Generator"
        content="Microsoft Word 15 (filtered medium)">
      <!--[if !mso]><style>v\:* {behavior:url(#default#VML);}
o\:* {behavior:url(#default#VML);}
w\:* {behavior:url(#default#VML);}
.shape {behavior:url(#default#VML);}
</style><![endif]-->
      <style>@font-face
        {font-family:"Cambria Math";
        panose-1:2 4 5 3 5 4 6 3 2 4;}@font-face
        {font-family:Calibri;
        panose-1:2 15 5 2 2 2 4 3 2 4;}@font-face
        {font-family:Aptos;}@font-face
        {font-family:wf_segoe-ui_normal;}@font-face
        {font-family:"Helvetica Neue";}p.MsoNormal, li.MsoNormal, div.MsoNormal
        {margin:0cm;
        font-size:10.0pt;
        font-family:"Aptos",sans-serif;}a:link, span.MsoHyperlink
        {mso-style-priority:99;
        color:blue;
        text-decoration:underline;}span.EmailStyle21
        {mso-style-type:personal-reply;
        font-family:"Aptos",sans-serif;
        color:windowtext;}.MsoChpDefault
        {mso-style-type:export-only;
        font-size:10.0pt;
        mso-ligatures:none;}div.WordSection1
        {page:WordSection1;}</style><!--[if gte mso 9]><xml>
<o:shapedefaults v:ext="edit" spidmax="1026" />
</xml><![endif]--><!--[if gte mso 9]><xml>
<o:shapelayout v:ext="edit">
<o:idmap v:ext="edit" data="1" />
</o:shapelayout></xml><![endif]-->
      <table style="border-collapse: collapse; padding-left: 0px;">
        <tbody>
          <tr>
            <td><font
style="font-family: Arial, sans-serif; font-size: 12px; font-style: normal; font-weight: normal; color: #000000; background-color: #FFECB3; line-height: 1.6; padding: 3px;">[<strong>CAUTION:</strong>
                Non-UBC Email]</font></td>
          </tr>
        </tbody>
      </table>
      <div class="WordSection1">
        <p class="MsoNormal"><span
            style="font-size:11.0pt;mso-fareast-language:EN-US">   It’s
            interesting to see such a wide variety of experiences. I’m
            too chicken to evaporate right out of the pocket, so we went
            through a lot of liners, too, before settling on something.
            <o:p></o:p></span></p>
        <p class="MsoNormal"><span
            style="font-size:11.0pt;mso-fareast-language:EN-US"><o:p> </o:p></span></p>
        <p class="MsoNormal"><span
            style="font-size:11.0pt;mso-fareast-language:EN-US">   We
            have had good luck with Cu liners for Ni e-beam evaporation,
            but with a 2.2 cc pocket, we have to be very careful to keep
            the beam away from the walls and limit the deposition rate
            to 1 Angstrom/s.<o:p></o:p></span></p>
        <p class="MsoNormal"><span
            style="font-size:11.0pt;mso-fareast-language:EN-US"><o:p> </o:p></span></p>
        <p class="MsoNormal"><span
            style="font-size:11.0pt;mso-fareast-language:EN-US">  Hope
            you find something that works, liners get expensive!<o:p></o:p></span></p>
        <p class="MsoNormal"><span
            style="font-size:11.0pt;mso-fareast-language:EN-US"><o:p> </o:p></span></p>
        <p class="MsoNormal"><span style="font-size:11.0pt"><o:p> </o:p></span></p>
        <p class="MsoNormal"><span lang="EN-US" style="font-size:11.0pt">Graham
            Gibson<o:p></o:p></span></p>
        <p class="MsoNormal"><span lang="EN-US" style="font-size:11.0pt"><o:p> </o:p></span></p>
        <p class="MsoNormal"><span lang="EN-US" style="font-size:9.0pt">Operations
            Manager, NanoFabrication Kingston<o:p></o:p></span></p>
        <p class="MsoNormal"><span lang="EN-US" style="font-size:9.0pt">Queen’s
            University<o:p></o:p></span></p>
        <p class="MsoNormal"><span lang="EN-US" style="font-size:9.0pt">945
            Princess Street<o:p></o:p></span></p>
        <p class="MsoNormal"><span lang="EN-US" style="font-size:9.0pt">Kingston,
            Ontario, Canada<o:p></o:p></span></p>
        <p class="MsoNormal"><span lang="EN-US" style="font-size:9.0pt">K7L
            0E9<o:p></o:p></span></p>
        <p class="MsoNormal"><span lang="EN-US" style="font-size:9.0pt"><a
              href="mailto:gibsong@queensu.ca" moz-do-not-send="true"><span
                style="color:#0563C1">gibsong@queensu.ca</span></a><o:p></o:p></span></p>
        <p class="MsoNormal"><span lang="EN-US" style="font-size:9.0pt"><a
              href="http://www.nanofabkingston.ca/"
              moz-do-not-send="true"><span style="color:#0563C1">www.nanofabkingston.ca</span></a><o:p></o:p></span></p>
        <p class="MsoNormal"><span style="font-size:11.0pt"><o:p> </o:p></span></p>
        <p class="MsoNormal"><span
            style="font-size:11.0pt;mso-fareast-language:EN-US"><o:p> </o:p></span></p>
        <p class="MsoNormal"><span
            style="font-size:11.0pt;mso-fareast-language:EN-US"><o:p> </o:p></span></p>
        <div>
          <div
style="border:none;border-top:solid #E1E1E1 1.0pt;padding:3.0pt 0cm 0cm 0cm">
            <p class="MsoNormal"><b><span lang="EN-US"
style="font-size:11.0pt;font-family:"Calibri",sans-serif">From:</span></b><span
                lang="EN-US"
style="font-size:11.0pt;font-family:"Calibri",sans-serif">
                labnetwork <a class="moz-txt-link-rfc2396E" href="mailto:labnetwork-bounces@mtl.mit.edu"><labnetwork-bounces@mtl.mit.edu></a>
                <b>On Behalf Of </b>Owain Clark<br>
                <b>Sent:</b> December 5, 2024 3:48 AM<br>
                <b>To:</b> Jeff Salzmann <a class="moz-txt-link-rfc2396E" href="mailto:jks7@buffalo.edu"><jks7@buffalo.edu></a>;
                Bernhard Reineke
                <a class="moz-txt-link-rfc2396E" href="mailto:bernhard.reineke@uni-paderborn.de"><bernhard.reineke@uni-paderborn.de></a>; shokoofe
                haghighi <a class="moz-txt-link-rfc2396E" href="mailto:shokoofe_haghighi@yahoo.com"><shokoofe_haghighi@yahoo.com></a>;
                <a class="moz-txt-link-abbreviated" href="mailto:labnetwork@mtl.mit.edu">labnetwork@mtl.mit.edu</a><br>
                <b>Subject:</b> Re: [labnetwork] question about Liner
                for Ni Ebeam Evaporation<o:p></o:p></span></p>
          </div>
        </div>
        <p class="MsoNormal"><o:p> </o:p></p>
        <p class="MsoNormal"><span lang="EN-GB"
            style="font-size:11.0pt;mso-fareast-language:EN-US">Interestingly
            we have no trouble with Ni, it is one of our most stable
            materials and the crucible has not been changed in years. I
            believe it is W.
            <o:p></o:p></span></p>
        <p class="MsoNormal"><span lang="EN-GB"
            style="font-size:11.0pt;mso-fareast-language:EN-US"><o:p> </o:p></span></p>
        <p class="MsoNormal"><span lang="EN-GB"
            style="font-size:11.0pt;mso-fareast-language:EN-US">I
            suspect reading these comments it is because we have larger
            40cc crucibles and we only melt a spot in the center with a
            small beam deflection. The crucible walls never see melted
            Ni. <o:p></o:p></span></p>
        <p class="MsoNormal"><span lang="EN-GB"
            style="font-size:11.0pt;mso-fareast-language:EN-US"><o:p> </o:p></span></p>
        <p class="MsoNormal"><span lang="EN-GB"
            style="font-size:11.0pt;mso-fareast-language:EN-US">BR,
            Owain<o:p></o:p></span></p>
        <p class="MsoNormal"><span lang="EN-GB"
            style="font-size:11.0pt;mso-fareast-language:EN-US"><o:p> </o:p></span></p>
        <div>
          <div
style="border:none;border-top:solid #E1E1E1 1.0pt;padding:3.0pt 0cm 0cm 0cm">
            <p class="MsoNormal"><b><span lang="EN-US"
style="font-size:11.0pt;font-family:"Calibri",sans-serif">From:</span></b><span
                lang="EN-US"
style="font-size:11.0pt;font-family:"Calibri",sans-serif">
                labnetwork <<a
                  href="mailto:labnetwork-bounces@mtl.mit.edu"
                  moz-do-not-send="true" class="moz-txt-link-freetext">labnetwork-bounces@mtl.mit.edu</a>>
                <b>On Behalf Of </b>Jeff Salzmann<br>
                <b>Sent:</b> 04 December 2024 17:15<br>
                <b>To:</b> Bernhard Reineke <<a
                  href="mailto:bernhard.reineke@uni-paderborn.de"
                  moz-do-not-send="true" class="moz-txt-link-freetext">bernhard.reineke@uni-paderborn.de</a>>;
                shokoofe haghighi <<a
                  href="mailto:shokoofe_haghighi@yahoo.com"
                  moz-do-not-send="true" class="moz-txt-link-freetext">shokoofe_haghighi@yahoo.com</a>>;
                <a href="mailto:labnetwork@mtl.mit.edu"
                  moz-do-not-send="true" class="moz-txt-link-freetext">labnetwork@mtl.mit.edu</a><br>
                <b>Subject:</b> Re: [labnetwork] question about Liner
                for Ni Ebeam Evaporation<o:p></o:p></span></p>
          </div>
        </div>
        <p class="MsoNormal"><span lang="EN-GB"><o:p> </o:p></span></p>
        <table class="MsoNormalTable" border="0" cellspacing="0"
          cellpadding="0" align="left" width="100%" style="width:100.0%">
          <tbody>
            <tr>
              <td width="0"
style="width:.3pt;background:#A6A6A6;padding:5.25pt 1.5pt 5.25pt 1.5pt">
                <br>
              </td>
              <td width="100%"
style="width:100.0%;background:#EAEAEA;padding:5.25pt 3.75pt 5.25pt 11.25pt;aspect-ratio: revert !important;background:revert !important;block-size: revert !important;border:revert !important;bottom: revert !important;color:revert !important;color-scheme: revert !important;content-visibility: revert !important;cursor:revert !important;direction:revert !important;display:revert !important;font-size:revert !important;height:revert !important;hyphens: revert !important;letter-spacing:revert !important;line-height:revert !important;margin:revert !important;opacity: revert !important;order: revert !important;outline: revert !important;overflow:revert !important;padding:revert !important;position:revert !important;resize: revert !important;rotate: revert !important;scale: revert !important;tab-size: revert !important;table-layout:revert !important;text-align:revert !important;text-indent:revert !important;text-orientation: revert !important;text-overflow: revert !important;text-shadow:revert !important;text-transform:revert !important;text-wrap: revert !important;top:revert !important;transition: revert !important;user-select: revert !important;vertical-align:revert !important;visibility:revert !important;white-space:revert !important;width:revert !important;word-break:revert !important;word-spacing:revert !important;writing-mode:revert !important;zoom: revert !important">
                <div>
                  <p class="MsoNormal"
style="mso-element:frame;mso-element-frame-hspace:2.25pt;mso-element-wrap:around;mso-element-anchor-vertical:paragraph;mso-element-anchor-horizontal:column;mso-height-rule:exactly">
                    <span
style="font-size:9.0pt;font-family:wf_segoe-ui_normal;color:#212121">You
                      don't often get email from
                      <a href="mailto:jks7@buffalo.edu"
                        moz-do-not-send="true"
                        class="moz-txt-link-freetext">jks7@buffalo.edu</a>.
                      <a
href="https://aka.ms/LearnAboutSenderIdentification"
                        moz-do-not-send="true">
                        Learn why this is important</a> <o:p></o:p></span></p>
                </div>
              </td>
              <td width="75"
style="width:56.25pt;background:#EAEAEA;padding:5.25pt 3.75pt 5.25pt 3.75pt;aspect-ratio: revert !important;background:revert !important;block-size: revert !important;border:revert !important;bottom: revert !important;color:revert !important;color-scheme: revert !important;content-visibility: revert !important;cursor:revert !important;direction:revert !important;display:revert !important;font-size:revert !important;height:revert !important;hyphens: revert !important;letter-spacing:revert !important;line-height:revert !important;margin:revert !important;opacity: revert !important;order: revert !important;outline: revert !important;overflow:revert !important;padding:revert !important;position:revert !important;resize: revert !important;rotate: revert !important;scale: revert !important;tab-size: revert !important;table-layout:revert !important;text-align:revert !important;text-indent:revert !important;text-orientation: revert !important;text-overflow: revert !important;text-shadow:revert !important;text-transform:revert !important;text-wrap: revert !important;top:revert !important;transition: revert !important;user-select: revert !important;vertical-align:revert !important;visibility:revert !important;white-space:revert !important;width:revert !important;word-break:revert !important;word-spacing:revert !important;writing-mode:revert !important;zoom: revert !important;align: left !important">
                <br>
              </td>
            </tr>
          </tbody>
        </table>
        <div>
          <div>
            <div
style="border:solid #8D3970 1.0pt;padding:9.0pt 9.0pt 9.0pt 9.0pt">
              <p class="MsoNormal"
                style="line-height:16.5pt;background:#F7F9FA"><strong><span
                    lang="EN-US"
style="font-size:10.5pt;font-family:"Calibri",sans-serif;color:#8D3970">CAUTION:</span></strong><span
                  lang="EN-US"
style="font-size:10.5pt;font-family:"Calibri",sans-serif;color:#8D3970">
                  This e-mail originated outside the University of
                  Southampton. <o:p></o:p></span></p>
            </div>
          </div>
          <div>
            <p class="MsoNormal"><span lang="EN-US"
                style="font-size:12.0pt">Haghighi,<o:p></o:p></span></p>
            <p class="MsoNormal"><span lang="EN-US"
                style="font-size:12.0pt"><o:p> </o:p></span></p>
            <p class="MsoNormal"><span lang="EN-US"
                style="font-size:12.0pt">This is my collection of failed
                crucibles used to evaporate Ni.
                <o:p></o:p></span></p>
            <p class="MsoNormal"><span lang="EN-US"
                style="font-size:12.0pt"><o:p> </o:p></span></p>
            <p class="MsoNormal"><span lang="EN-US"
                style="font-size:12.0pt">We decided on graphite, because
                copper was worse. We limit our deposition rate to 0.2</span><span
                lang="EN-US"
style="font-size:10.5pt;font-family:"Arial",sans-serif;color:black;background:#F8F9FA">
              </span><span lang="EN-US" style="font-size:12.0pt">Å/sec
                to help extend the lifespan of the crucibles. They still
                fail after 2-3 depositions.<o:p></o:p></span></p>
            <p class="MsoNormal"><span lang="EN-US"
                style="font-size:12.0pt"><o:p> </o:p></span></p>
            <p class="MsoNormal"><span lang="EN-US"
                style="font-size:12.0pt">Regards,<o:p></o:p></span></p>
            <p class="MsoNormal"><span lang="EN-US"
                style="font-size:12.0pt">Jeff<o:p></o:p></span></p>
            <p class="MsoNormal"><span lang="EN-US"
                style="font-size:12.0pt"><o:p> </o:p></span></p>
            <p class="MsoNormal"><span lang="EN-US"
                style="font-size:12.0pt"><o:p> </o:p></span></p>
            <div>
              <div>
                <p class="MsoNormal"><span lang="EN-US"
style="font-size:11.0pt;font-family:"Calibri",sans-serif;color:black">Jeff
                    Salzmann</span><span lang="EN-US"
                    style="font-size:11.0pt;color:black"><o:p></o:p></span></p>
                <p class="MsoNormal"><span lang="EN-US"
style="font-size:11.0pt;font-family:"Calibri",sans-serif;color:black">Assistant
                    Professor of Research</span><span lang="EN-US"
                    style="font-size:11.0pt;color:black"><o:p></o:p></span></p>
                <p class="MsoNormal"><span lang="EN-US"
style="font-size:11.0pt;font-family:"Calibri",sans-serif;color:black">Cleanroom
                    Manager, Shared Instrumentation Laboratories</span><span
                    lang="EN-US" style="font-size:11.0pt;color:black"><o:p></o:p></span></p>
                <p class="MsoNormal"><span lang="EN-US"
style="font-size:11.0pt;font-family:"Calibri",sans-serif;color:black">School
                    of Engineering and Applied Sciences</span><span
                    lang="EN-US" style="font-size:11.0pt;color:black"><o:p></o:p></span></p>
                <p class="MsoNormal"><span lang="EN-US"
style="font-size:11.0pt;font-family:"Calibri",sans-serif;color:black">University
                    at Buffalo</span><span lang="EN-US"
                    style="font-size:11.0pt;color:black"><o:p></o:p></span></p>
                <p class="MsoNormal"><span lang="EN-US"
style="font-size:11.0pt;font-family:"Calibri",sans-serif;color:black">114A
                    Davis Hall</span><span lang="EN-US"
                    style="font-size:11.0pt;color:black"><o:p></o:p></span></p>
                <p class="MsoNormal"><span lang="EN-US"
style="font-size:11.0pt;font-family:"Calibri",sans-serif;color:black">Buffalo,
                    NY 14260</span><span lang="EN-US"
                    style="font-size:11.0pt;color:black"><o:p></o:p></span></p>
                <p class="MsoNormal"><span lang="EN-US"
style="font-size:11.0pt;font-family:"Calibri",sans-serif;color:black">Tel:
                    716.645.2584</span><span lang="EN-US"
                    style="font-size:11.0pt;color:black"><o:p></o:p></span></p>
              </div>
            </div>
            <p class="MsoNormal"><span lang="EN-US"
                style="font-size:12.0pt"><o:p> </o:p></span></p>
            <div id="mail-editor-reference-message-container">
              <div>
                <div>
                  <div
style="border:none;border-top:solid #B5C4DF 1.0pt;padding:3.0pt 0cm 0cm 0cm">
                    <p class="MsoNormal" style="margin-bottom:12.0pt"><b><span
                          lang="EN-US"
                          style="font-size:12.0pt;color:black">From:
                        </span></b><span lang="EN-US"
                        style="font-size:12.0pt;color:black">labnetwork
                        <<a
                          href="mailto:labnetwork-bounces@mtl.mit.edu"
                          moz-do-not-send="true"
                          class="moz-txt-link-freetext">labnetwork-bounces@mtl.mit.edu</a>>
                        on behalf of Bernhard Reineke <<a
href="mailto:bernhard.reineke@uni-paderborn.de" moz-do-not-send="true"
                          class="moz-txt-link-freetext">bernhard.reineke@uni-paderborn.de</a>><br>
                        <b>Date: </b>Wednesday, December 4, 2024 at
                        11:46<br>
                        <b>To: </b>shokoofe haghighi <<a
                          href="mailto:shokoofe_haghighi@yahoo.com"
                          moz-do-not-send="true"
                          class="moz-txt-link-freetext">shokoofe_haghighi@yahoo.com</a>>,
                        <a href="mailto:labnetwork@mtl.mit.edu"
                          moz-do-not-send="true"
                          class="moz-txt-link-freetext">labnetwork@mtl.mit.edu</a>
                        <<a href="mailto:labnetwork@mtl.mit.edu"
                          moz-do-not-send="true"
                          class="moz-txt-link-freetext">labnetwork@mtl.mit.edu</a>><br>
                        <b>Subject: </b>Re: [labnetwork] question about
                        Liner for Ni Ebeam Evaporation<o:p></o:p></span></p>
                  </div>
                  <table class="MsoNormalTable" border="0"
                    cellspacing="0" cellpadding="0" align="left"
                    width="100%"
style="width:100.0%;background:revert!important;border:revert!important;bottom:revert!important;color:revert!important;direction:revert!important;display:revert!important;font-size:revert!important;height:revert!important;letter-spacing:revert!important;line-height:revert!important;margin:revert!important;opacity:revert!important;order:revert!important;outline:revert!important;overflow:revert!important;padding:revert!important;position:revert!important;tab-size:revert!important;table-layout:revert!important;text-align:revert!important;text-indent:revert!important;text-orientation:revert!important;text-overflow:revert!important;text-transform:revert!important;top:revert!important;vertical-align:revert!important;visibility:revert!important;white-space:revert!important;width:revert!important;word-break:revert!important;word-spacing:revert!important;writing-mode:revert!important;zoom:revert!important;border:0!important;display:table!important;width:100%!important;table-layout:fixed!important;border-collapse:seperate!important;float:none!important;border-spacing:0px 0px!important">
                    <tbody>
                      <tr
style="background:revert!important;border:revert!important;bottom:revert!important;color:revert!important;direction:revert!important;display:revert!important;font-size:revert!important;height:revert!important;letter-spacing:revert!important;line-height:revert!important;margin:revert!important;opacity:revert!important;order:revert!important;outline:revert!important;overflow:revert!important;padding:revert!important;position:revert!important;tab-size:revert!important;table-layout:revert!important;text-align:revert!important;text-indent:revert!important;text-orientation:revert!important;text-overflow:revert!important;text-transform:revert!important;top:revert!important;vertical-align:revert!important;visibility:revert!important;white-space:revert!important;width:revert!important;word-break:revert!important;word-spacing:revert!important;writing-mode:revert!important;zoom:revert!important">
                        <td
style="background:#A6A6A6;padding:0cm 0cm 0cm 0cm;background:revert!important;border:revert!important;bottom:revert!important;color:revert!important;direction:revert!important;display:revert!important;font-size:revert!important;height:revert!important;letter-spacing:revert!important;line-height:revert!important;margin:revert!important;opacity:revert!important;order:revert!important;outline:revert!important;overflow:revert!important;padding:revert!important;position:revert!important;tab-size:revert!important;table-layout:revert!important;text-align:revert!important;text-indent:revert!important;text-orientation:revert!important;text-overflow:revert!important;text-transform:revert!important;top:revert!important;vertical-align:revert!important;visibility:revert!important;white-space:revert!important;width:revert!important;word-break:revert!important;word-spacing:revert!important;writing-mode:revert!important;zoom:revert!important;padding:2px!important;background-color:#A6A6A6!important;width:0px!important">
                          <br>
                        </td>
                        <td width="100%"
style="width:100.0%;background:#EAEAEA;padding:0cm 0cm 0cm 0cm;background:revert!important;border:revert!important;bottom:revert!important;color:revert!important;direction:revert!important;display:revert!important;font-size:revert!important;height:revert!important;letter-spacing:revert!important;line-height:revert!important;margin:revert!important;opacity:revert!important;order:revert!important;outline:revert!important;overflow:revert!important;padding:revert!important;position:revert!important;tab-size:revert!important;table-layout:revert!important;text-align:revert!important;text-indent:revert!important;text-orientation:revert!important;text-overflow:revert!important;text-transform:revert!important;top:revert!important;vertical-align:revert!important;visibility:revert!important;white-space:revert!important;width:revert!important;word-break:revert!important;word-spacing:revert!important;writing-mode:revert!important;zoom:revert!important;width:100%!important;background-color:#EAEAEA!important;padding:15px!important;font-size:12px!important;font-weight:normal!important;color:#212121!important;text-align:left!important;word-wrap:break-word!important">
                          <div>
                            <p class="MsoNormal"
style="mso-element:frame;mso-element-frame-hspace:2.25pt;mso-element-wrap:around;mso-element-anchor-vertical:paragraph;mso-element-anchor-horizontal:column;mso-height-rule:exactly">
                              <span
style="font-size:12.0pt;font-family:wf_segoe-ui_normal;color:black">You
                                don't often get email from
                                <a
href="mailto:bernhard.reineke@uni-paderborn.de" moz-do-not-send="true"
                                  class="moz-txt-link-freetext">bernhard.reineke@uni-paderborn.de</a>.
                                <a
href="https://aka.ms/LearnAboutSenderIdentification"
                                  moz-do-not-send="true">Learn why this
                                  is important</a>
                              </span><span
style="font-size:12.0pt;font-family:wf_segoe-ui_normal"><o:p></o:p></span></p>
                          </div>
                        </td>
                        <td
style="background:#EAEAEA;padding:0cm 0cm 0cm 0cm;background:revert!important;border:revert!important;bottom:revert!important;color:revert!important;direction:revert!important;display:revert!important;font-size:revert!important;height:revert!important;letter-spacing:revert!important;line-height:revert!important;margin:revert!important;opacity:revert!important;order:revert!important;outline:revert!important;overflow:revert!important;padding:revert!important;position:revert!important;tab-size:revert!important;table-layout:revert!important;text-align:revert!important;text-indent:revert!important;text-orientation:revert!important;text-overflow:revert!important;text-transform:revert!important;top:revert!important;vertical-align:revert!important;visibility:revert!important;white-space:revert!important;width:revert!important;word-break:revert!important;word-spacing:revert!important;writing-mode:revert!important;zoom:revert!important;width:75px!important;background-color:#EAEAEA!important;padding:5px!important;font-size:12px!important;font-weight:normal!important;color:#212121!important;text-align:left!important;word-wrap:break-word!important">
                          <br>
                        </td>
                      </tr>
                    </tbody>
                  </table>
                  <div>
                    <p class="MsoNormal"><span lang="EN-US"
                        style="font-size:12.0pt">Hi Haghighi,<br>
                        <br>
                        we tried this once, same result. All liners will
                        crack. Lesker has some recommendations on Ebeam
                        evaporation of Ni: slow power ramp up and down
                        (works well to prevent cracking for ~2-4 Runs,
                        with fabmate). A Cu liner should work better but
                        we never tested that.<br>
                        <br>
                        <a
href="https://www.lesker.com/newweb/deposition_materials/depositionmaterials_evaporationmaterials_1.cfm?pgid=ni1"
                          moz-do-not-send="true"
                          class="moz-txt-link-freetext">https://www.lesker.com/newweb/deposition_materials/depositionmaterials_evaporationmaterials_1.cfm?pgid=ni1</a><br>
                        <br>
                        Best,<br>
                        <br>
                        Bernhard <o:p></o:p></span></p>
                    <div class="MsoNormal" align="center"
                      style="text-align:center"><span lang="EN-US"
                        style="font-size:12.0pt">
                        <hr size="1" width="100%" align="center">
                      </span></div>
                    <div id="divRplyFwdMsg">
                      <p class="MsoNormal"><b><span lang="EN-US"
style="font-size:11.0pt;font-family:"Calibri",sans-serif;color:black">Von:</span></b><span
                          lang="EN-US"
style="font-size:11.0pt;font-family:"Calibri",sans-serif;color:black">
                          labnetwork <<a
                            href="mailto:labnetwork-bounces@mtl.mit.edu"
                            moz-do-not-send="true"
                            class="moz-txt-link-freetext">labnetwork-bounces@mtl.mit.edu</a>>
                          im Auftrag von shokoofe haghighi <<a
                            href="mailto:shokoofe_haghighi@yahoo.com"
                            moz-do-not-send="true"
                            class="moz-txt-link-freetext">shokoofe_haghighi@yahoo.com</a>><br>
                          <b>Gesendet:</b> Mittwoch, 4. Dezember 2024
                          10:35:19<br>
                          <b>An:</b> <a
                            href="mailto:labnetwork@mtl.mit.edu"
                            moz-do-not-send="true"
                            class="moz-txt-link-freetext">labnetwork@mtl.mit.edu</a><br>
                          <b>Betreff:</b> [labnetwork] question about
                          Liner for Ni Ebeam Evaporation</span><span
                          lang="EN-US" style="font-size:12.0pt">
                          <o:p></o:p></span></p>
                      <div>
                        <p class="MsoNormal"><span lang="EN-US"
                            style="font-size:12.0pt"> <o:p></o:p></span></p>
                      </div>
                    </div>
                    <div>
                      <div>
                        <div>
                          <p class="MsoNormal"><span lang="EN-US"
style="font-family:"Helvetica Neue"">Hi, hope you are having
                              good days, <o:p></o:p></span></p>
                        </div>
                        <div>
                          <p class="MsoNormal"><span lang="EN-US"
style="font-family:"Helvetica Neue""><o:p> </o:p></span></p>
                        </div>
                        <div>
                          <p class="MsoNormal"><span lang="EN-US"
style="font-family:"Helvetica Neue"">this is Haghighi, working
                              on metallization by a PVD, using thermal
                              and Ebeam evaporation. <o:p></o:p></span></p>
                        </div>
                        <div>
                          <p class="MsoNormal"><span lang="EN-US"
style="font-family:"Helvetica Neue""><o:p> </o:p></span></p>
                        </div>
                        <div>
                          <p class="MsoNormal"><span lang="EN-US"
style="font-family:"Helvetica Neue"">I have some issues
                              choosing the right liner for Ni Ebeam
                              evaporating, hope you find time to guide
                              me through it.  <o:p></o:p></span></p>
                        </div>
                        <div>
                          <p class="MsoNormal"><span lang="EN-US"
style="font-family:"Helvetica Neue"">We have tested graphite,
                              glassy carbon coated graphite, Al2O3, Mo,
                              W and Cu liners so far. <o:p></o:p></span></p>
                        </div>
                        <div>
                          <p class="MsoNormal"><span lang="EN-US"
style="font-family:"Helvetica Neue"">    Graphite liner just
                              broke after first run from the border line
                              of Ni surface. <span style="color:black">Glassy
                                carbon coated graphite was more or less
                                the same,</span><o:p></o:p></span></p>
                        </div>
                        <div>
                          <p class="MsoNormal"><span lang="EN-US"
style="font-family:"Helvetica Neue"">    Al2O3 endured for 4-5
                              runs before breaking but there were cracks
                              on it,  <o:p></o:p></span></p>
                        </div>
                        <div>
                          <p class="MsoNormal"><span lang="EN-US"
style="font-family:"Helvetica Neue"">    Mo liner totally
                              melted and some kind of alloy was
                              produced,<o:p></o:p></span></p>
                        </div>
                        <div>
                          <p class="MsoNormal"><span lang="EN-US"
style="font-family:"Helvetica Neue"">    W and Cu endured but
                              their internal walls were some how melted
                              and we can't be sure about pureness of
                              evaporated Ni and final produced thin
                              films.<o:p></o:p></span></p>
                        </div>
                        <div>
                          <p class="MsoNormal"><span lang="EN-US"
style="font-family:"Helvetica Neue""><o:p> </o:p></span></p>
                        </div>
                        <div>
                          <p class="MsoNormal"><span lang="EN-US"
style="font-family:"Helvetica Neue"">do you have any other
                              suggestions? <o:p></o:p></span></p>
                        </div>
                        <div>
                          <p class="MsoNormal"><span lang="EN-US"
style="font-family:"Helvetica Neue""><o:p> </o:p></span></p>
                        </div>
                        <div>
                          <p class="MsoNormal"><span lang="EN-US"
style="font-family:"Helvetica Neue""><o:p> </o:p></span></p>
                        </div>
                        <div>
                          <p class="MsoNormal"><span lang="EN-US"
style="font-family:"Helvetica Neue"">high voltage: 6.1 KV<o:p></o:p></span></p>
                        </div>
                        <div>
                          <p class="MsoNormal"><span lang="EN-US"
style="font-family:"Helvetica Neue"">emission current: 3 - 5 A<o:p></o:p></span></p>
                        </div>
                        <div>
                          <p class="MsoNormal"><span lang="EN-US"
style="font-family:"Helvetica Neue""><o:p> </o:p></span></p>
                        </div>
                        <div>
                          <p class="MsoNormal"><span lang="EN-US"
style="font-family:"Helvetica Neue"">    <o:p></o:p></span></p>
                        </div>
                        <div>
                          <p class="MsoNormal"><span lang="EN-US"
style="font-family:"Helvetica Neue"">Thanks for your time and
                              attention in advance, I hope you kindly
                              find time and consider replying me,  <o:p></o:p></span></p>
                        </div>
                        <div>
                          <p class="MsoNormal"><span lang="EN-US"
style="font-family:"Helvetica Neue""><o:p> </o:p></span></p>
                        </div>
                        <div>
                          <p class="MsoNormal"><span lang="EN-US"
style="font-family:"Helvetica Neue"">Dr. Haghighi<o:p></o:p></span></p>
                        </div>
                        <div>
                          <p class="MsoNormal"><span lang="EN-US"
style="font-family:"Helvetica Neue""><o:p> </o:p></span></p>
                        </div>
                      </div>
                    </div>
                  </div>
                </div>
              </div>
            </div>
          </div>
        </div>
      </div>
      <br>
      <fieldset class="moz-mime-attachment-header"></fieldset>
      <pre wrap="" class="moz-quote-pre">_______________________________________________
labnetwork mailing list
<a class="moz-txt-link-abbreviated" href="mailto:labnetwork@mtl.mit.edu">labnetwork@mtl.mit.edu</a>
<a class="moz-txt-link-freetext" href="https://mtl.mit.edu/mailman/listinfo.cgi/labnetwork">https://mtl.mit.edu/mailman/listinfo.cgi/labnetwork</a>
</pre>
    </blockquote>
    <div class="moz-signature">-- <br>
      <img src="cid:part1.wgbSFHy6.NFPajvYu@physics.ubc.ca" border="0"></div>
  </body>
</html>