Dear Vito,
I wonder what you mean with precision cleaving. We use to cleave GaN/sapphire using a classic diamond scribing tool. We do full line scribe and pass the diamond tool several time on the sapphire side. Then we flip the wafer upside down on a rubber mat (mouse pad) and place a SS 2mm diameter rod and we push on both sides of the rod and generally increasing the pressure till it breaks.
We were not interested in the shape of the cleave but and I don't believe you can get a vertical smooth wall as the cleavage is not relying on a cleavage plan (which is not straightforward with sapphire).
For precision cleaving I know Loomis industry in California developed a scriber tool for sapphire based on full line scribe followed by a roller (like Espen described) to break the wafer.
Hope this helps,
Fouad Karouta
*********************************
Manager ANFF ACT Node
Australian National Fabrication Facility
Research School of Physics and Engineering
L. Huxley Building (#56), Mills Road, Room 4.02
Australian National University
ACT 0200, Canberra, Australia
Tel: + 61 2 6125 7174
Mob: + 61 451 046 412
Email: fouad.karouta at anu.edu.au<mailto:fouad.karouta at anu.edu.au>
http://anff-act.anu.edu.au/
From: labnetwork-bounces at mtl.mit.edu [mailto:labnetwork-bounces at mtl.mit.edu] On Behalf Of Espen Rogstad
Sent: Sunday, November 8, 2015 4:17 AM
To: Vito Logiudice
Cc: labnetwork at mtl.mit.edu
Subject: Re: [labnetwork] Sapphire substrates: precision scribe & break
Hi Vito,
A couple of years ago we scribed and cleaved a few 2" sapphire wafers that were around 300um thick. This was done with a dynatex II scribe & break machine that I guess is around 15 years old. Had to use quite high scribing and breaking force (I can check numbers if interested) but it worked fine. The diamond scribe tool would probably not last very long but since we only scribed a few wafers we didn't have any issues with that. Also, never checked sidewalls so don't know if they were smooth or not... Hope this helps anyway!
Regards,
Espen Rogstad
Senior Engineer
NTNU NanoLab
-------------------------
Sem Sælands vei 14, K1-113
NO-7491 Trondheim, Norway
Tlf: +47 95285642
http://www.ntnu.no/nanolab
Den 7. nov. 2015 kl. 15.17 skrev Christopher Raum <crraum at gmail.com<mailto:crraum at gmail.com>>:
Hi Vito,
I've had success scribing across the length of the desired cleave location and then using the length of a hex key (1 to 2 mm) to provide a fulcrum under the scribe line. Then by placing finger tips on either side of the scribe (freshly trimmed fingernails help), push down evenly over the hex key edge. By placing a gentle but steadily increasing pressure I've been able to successfully cleave fused quartz wafers (100 to 500 um thick) this way.
This technique is heavily operator dependent and not suitable for large volume, but if you just need some experimental samples prepared it's a useful technique.
Good luck!
-Chris
--
Christopher Raum, PhD.
R&D Engineer
Experimental Cosmology Group
Radio Astronomy Lab
University of California, Berkeley
151 LeConte Hall
Berkeley, CA, 94720
Work: (510) 642-7801
Cell: (949) 677-1905
Fax: (510) 643-5204
Email: craum at berkeley.edu<mailto:craum at berkeley.edu>
Alt Email: crraum at gmail.com<mailto:crraum at gmail.com>
On Fri, Nov 6, 2015 at 10:42 AM, Vito Logiudice <vito.logiudice at uwaterloo.ca<mailto:vito.logiudice at uwaterloo.ca>> wrote:
Dear Colleagues,
I would appreciate hearing from anyone whom might be able to share some insights on how to reliably scribe & break sapphire substrates. We're attempting to help out a couple of research groups here with such a requirement.
We've had success with our water-cooled dicing saw but it appears this approach leads to unacceptable materials issues. We thus find ourselves having to resort to some sort of precision (& repeatable) scribe and break technique/setup which will result in consistently smooth sidewalls.
Thank you for any insights on procedures you may be using or equipment vendors you have worked with whom might be able to help.
Best regards,
Vito
--
Vito Logiudice P.Eng.
Director of Operations, Quantum NanoFab
University of Waterloo
Lazaridis QNC 1207
200 University Avenue West
Waterloo, ON Canada N2L 3G1
Tel.: (519) 888-4567 ext. 38703<tel:%28519%29%20888-4567%20%C2%A0ext.%2038703>
Email: vito.logiudice at uwaterloo.ca<mailto:vito.logiudice at uwaterloo.ca>
Website: https://fab.qnc.uwaterloo.ca
_______________________________________________
labnetwork mailing list
labnetwork at mtl.mit.edu<mailto:labnetwork at mtl.mit.edu>
https://www-mtl.mit.edu/mailman/listinfo.cgi/labnetwork
_______________________________________________
labnetwork mailing list
labnetwork at mtl.mit.edu<mailto:labnetwork at mtl.mit.edu>
https://www-mtl.mit.edu/mailman/listinfo.cgi/labnetwork
-------------- next part --------------
An HTML attachment was scrubbed...
URL: <https://mtl.mit.edu/pipermail/labnetwork/attachments/20151108/c7e7a6fa/attachment.html>
More information about the labnetwork
mailing list